Technical Articles

Ball Pressure Test to IEC 60695-10-2: 20 N, One Hour and the 2 mm Dent

2026-11-16

The ball pressure test is one of the simplest heat resistance tests in electrical safety, and one of the most inconsistently performed. The apparatus is a steel ball, a weight and an oven. The result depends on where the ball sits, how the specimen is supported, how the specimen is cooled and where the dent is measured. Each of those is a place where two laboratories can reach different answers on the same moulding.

The conditions

IEC 60695-10-2 defines the method, and the numbers are few enough to state plainly:

BallSteel sphere, 5 mm diameter, polished
Load20 N applied through the ball to the specimen
Duration1 hour at test temperature
Temperature75 degrees C for parts not retaining current-carrying parts; 125 degrees C where they do
AcceptanceDent diameter not greater than 2 mm

The 75 and 125 degree pair is the part people get wrong at the specification stage. The higher temperature is not for "hot" parts but for parts that hold a current-carrying connection in position, because a deformed support there becomes a creepage or clearance failure rather than a cosmetic one.

Specimen support decides the answer

The ball presses the specimen against a support. If the support is softer than the standard expects, the specimen sinks into it and the apparent dent is smaller than reality. If the support is smaller than the specimen, the specimen bends and the dent is deeper. Three rules:

  • Support the specimen on a flat steel plate at least 3 mm thick.
  • Test the part as moulded, at the thickness it has in service. A 3 mm test plaque is not a substitute for a 1.5 mm rib.
  • Where the part is too small or too curved to sit flat, use the smallest area that still carries the ball without rocking, and record that choice.

Cooling is part of the method

The measurement of a dent in a thermoplastic is a measurement of recovered shape, and recovery depends on how the specimen is cooled. The method calls for the load to be removed and the specimen cooled in water at around 20 degrees C for about 6 minutes, then measured within a few minutes. Left to cool in air, a part continues to recover for ten minutes or more and the dent reads smaller.

The two errors that follow are common and opposite:

  1. Measured hot. A dent measured immediately after the oven reads larger, because the material is still soft and the ball has not been fully removed from the surface.
  2. Measured cold and late. A dent measured after an hour on the bench reads smaller, and a marginal fail becomes a pass.

Measuring the dent

The dimension is the diameter of the impression, measured in two directions at right angles, and the larger value is reported. A travelling microscope or a profile projector is the appropriate instrument; a steel rule across a dent has a resolution problem that is larger than the discrimination required.

Two practical notes:

  • Light the dent from the side. A dent lit from directly above has no visible edge and reads small.
  • Where the dent has a raised rim, measure the rim-to-rim diameter, not the flat bottom. The rim is material that has been displaced, and it is part of the deformation.

When the result is marginal

A 2.1 mm dent on a 75 degree C test is a fail, but it is worth understanding what it means before changing the material. Three causes, in order of frequency:

  1. The part is thinner than the qualification plaque. Thin sections heat faster and deform more. Re-test at service thickness before concluding anything about the resin.
  2. The support was inadequate. A part that bent under the ball shows a deeper dent than the same material tested flat.
  3. The material is genuinely marginal at that temperature. This is where a grade change or a design change is the answer, and it is the least common of the three.

A retest at the correct thickness and on a proper support is cheap. A material change based on a badly supported test is expensive and may not fix the problem.

Records worth keeping

Record the test temperature, the load, the ball diameter, the support used, the specimen thickness at the test point, the dent in two directions and the cooling time. Six months later, the only question anyone asks is whether the sample was representative, and the answer is in the thickness column.

The flammability and heat testing range covers ball pressure apparatus with calibrated loads and 5 mm balls; the main catalogue indexes the ovens and specimen supports used with it.

Contact Us

Contact: Eason Wang

Phone: +86-13751010017

Tel: +86-755-33168386

Add: 1F Junfeng Building, Gongle, Xixiang, Baoan District, Shenzhen, Guangdong, China

close
Scan the qr codeClose
the qr code