Salt Mist to IEC 60068-2-11: 5 % NaCl, 35 °C and the Duration You Actually Need

2026-11-17

Salt mist is the test everybody asks for and the test most often misread. A part that shows rust after 24 hours has not necessarily failed, and a part that shows nothing after 96 hours has not necessarily passed. The test produces a condition; the verdict comes from the product standard, and the two are frequently confused.

What the test does control precisely is the environment. Four parameters define it, and all four have to be recorded for the result to mean anything.

The four parameters

ParameterValueConsequence if wrong
Sodium chloride concentration5 % ± 1 % by massChanges corrosion rate non-linearly
Chamber temperature35 °C ± 2 KSets the reaction rate and the evaporation
pH of the solution6.5 to 7.2Acidic solution attacks far faster
Exposure duration24 h, 48 h or 96 h, by product standardDurations are not interchangeable
Salt deposition rateSet by the spray rate, checked by collectorsA dry fog is not a salt mist test
Angle of the specimen20 degrees from vertical, typicallyFlat surfaces pool and give false results

The deposition rate check is the one that separates a real chamber from a box with a nozzle. Collectors placed in the chamber must gather a specified volume per unit area per hour; if they do not, the chamber is running a humidity test with salty water, and the result will be optimistic.

Why the duration cannot be converted

Corrosion is not linear in time. A protective layer that forms in the first hours can slow attack, while a coating that fails at a defect will accelerate once the base metal is exposed. That is why 24 hours and 96 hours are different tests rather than two points on one curve, and why a supplier who reports "passed salt spray" without the duration has reported nothing.

The same applies to cycles. Continuous exposure and cyclic exposure (wet, dry, wet) produce different failure modes: continuous tends to general attack, cyclic tends to crevice and undercut attack at edges.

Preparing a specimen that gives a usable answer

  • Clean but do not polish. Solvent wipe removes handling oil; abrasion removes the very surface you are testing.
  • Do not seal edges unless the product seals them. A cut edge in a real assembly is exposed, and that is where corrosion starts.
  • Mark the orientation. The same part at 20 degrees and at horizontal will differ, and a photograph taken from an unrecorded angle proves nothing.
  • Photograph before and after, same lighting, same distance. Corrosion assessment is comparative.

Reading the result

Record the type of attack, not just its presence: white rust on zinc, red rust on steel, blistering of paint, creep of corrosion from a scribe. Measure the width of creep from a scribed line in millimetres, and the area fraction affected. Those two numbers are comparable between laboratories; "some corrosion" is not.

Then check the clause that applies. A product standard may allow red rust on 5 percent of the area after 48 hours and none after 24. Without that clause, a photograph and a duration are not a result. A salt mist chamber with calibrated collectors and a documented deposition rate is the minimum for a defensible report, and the site index lists the chambers by internal volume.

Standards referenced: IEC 60068-2-11; ISO 9227.

Contact Us

Contact: Eason Wang

Phone: +86-13751010017

Tel: +86-755-33168386

Add: 1F Junfeng Building, Gongle, Xixiang, Baoan District, Shenzhen, Guangdong, China

close
Scan the qr codeClose
the qr code